Vuam cov ntaub ntawv rau kev xaiv cov hlau (tib yam hlau)

Hlau No.

Hluav taws xob

SAW

GTAW

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Qauv

Lub khw kos npe

Lub khw kos npe

Q235-AF

qw 235a

E4303 j422 ua

H08A

HJ431 TIG-J 50
10 (pib)

20 (pib)

E4303 j422 ua

H08MnA

HJ431 TIG-J 50

Q235-B

Q235-C

E4316E4315 j426j427

H08A

H08 E

HJ431 TIG-J 50

20g, 20g

20R, 20 (Forging)

E4315E4315 j426j427

H08A

H08 E

H08MnA

HJ43I TIG-J 50

6 mn!

16 MnR

E5016E5015 j506j507

HlOMnSi

H10Mn 2

HJ431HJ350 HlOMnSi
16 MnD

I6MnDR

E5016-G

E5015-G

J506 RH

J507RH

HlOMnNiMoA

SJ 101 TG 50

15 MnNiDR

E5015-G

wb 607

H08MnA SJ 102 TG 50

 

CO2 Gas Weld

Vuam khoom kom qhuav Temp.

Roj

Hlau hlau No. (standard)

Roj

Ar

H08MnSi

CO2

75-150 C

(lh)

Ar

H08MnSi

CO2

75-150 ° C

(lh)

Ar

H08MnSi

CO2

35O-38O°C (lh)

Ar

H08MnSi

CO2

350-380C (lh)

Ar

H08Mn2 Si

CO2

35O-38OC (lh)

Ar

MG50-3

CO2

35O-38OC (lh)

Ar

MG49-Ni

CO2

35O-38OC (lh)

Hlau No.

Hluav taws xob

SAW

GTAW

CO2 Gas Weld

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe

12 CrMo

E5515-IB R207 H08CrMoA

HJ350

TIG-R 30

Ar H08CrMnSi

Mo

CO2 150-250 ° C 650-700 ° C

380-420C (1.5h)

15 CrMo

E5515-B2 R307 H13CrMoA

HJ350

SJ103

Qauv: ER55-B2

Tom ntej: ER55-B2L

Ar

ER55-G

CO2 I5O-25 ° C 650-700 NwseC

380 ~ 420 ° C (1.5h)

12 CrlMoV

E5515-B2-

V

R317

H08CrMoVA

HJ 35 O

ER55B2MnV

Ar 200-300 ° C 650-700 ° C

380 ~ 420 ° C (1.5h)

lCr5 mav

E5MoV 15 r507 ua

H0Cr5Mo

Ar 200-300 ° C 760 ± 10 ° C

380 ~ 420 ° C (1.5h)

0c8n 9

E308-16E308-I5 ib 02al07

H0Cr2INil0

HJ 260

H0Cr21Nil0 Ar

Al 02. Al 07 150 ° Ch 250 ° Ch

OCrl8NilOTi !Crl8Ni9Ti

E437-16E437-15 A132A137

H0Cr21Nil0T

i

HJ 260

H0Cr21NiI0T

i

Ar AI32.AI37150 ° Clh250 ° Ch

0Cr7Nil2Mo

2

E316-16E316-15 A202A207

H0Crl9NiI 2

Mo2

HJ 260

H0Crl9NiI2 Mo2

Ar

A202.A207

150 ° C h

250 ° C h

 

Hlau No.

Hluav taws xob

SAW

GTAW

CO2 Gas Weld

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe
0Cr8Nil2Mo2 E316L-16E318-16 A022A2I2

H00Cr9Ni

12 hmo 2

HJ 260

H00Cr9Ni

12 hmo 2

Ar

A022.A212

! 50° Cwj

00Cr9n0 E308L-16 A002

H00Cr21Nil0

HJ 260

H00Cr21Nil0

Ar

A002

150 ° C h

lcr! 3

E410-16 G202

G202

150° COJ

!Cr6Si2Mo

E5MoV 15

r507 ua

380 ~ 420 ° C (1.5h)

RQTSi505

EZC Z202

Z202

150 ° C h

Vuam cov ntaub ntawv rau kev xaiv cov hlau sib txawv (cov hlau tsis sib xws)

Hlau No.

Joint niam txiv cov ntaub ntawv qeb qeb los yog pab pawg naj npawb

Hluav taws xob

SAW

GTAW

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe

Vuam ntawm carbon steel

Kuv + I

E4303

j422 ua

H08A

HJ431

TIG-J 50

Ar

J422J427

150 ° C h

380 ° C h

E4315

j427 ua

Vuam ntawm carbon steel thiab high-strength low-alloy steel

Kuv + (H-1)

E4303

j422 ua

H08A

H08MnA

HJ431

HlOMnSi

Ar

J422J427

150 ° C h

380 ° C h

E4315

j427 ua

1+ (II+2)

E4315

j427 ua

H08MnA

HJ431

HlOMnSi

Ar

j427j507

E5016

j507 ua

380 ° C 1.5 hli

1+ (III+1.)1+ (III+ 2.) E43I5

j427 ua

H08AH08MnA HJ431 HlOMnSi Ar

j427j507

380 ° C 1.5 hli

E5015

j507 ua

Vuam ntawm carbon steel thiab tshav kub-resistant low alloy steel

I + IV E4315

j427 ua

H08A

H08MnA

HJ431

HlOMnSi Ar

150-250 ° C

650-700 ° C

j427 ua

380 ° C 1.5 hli

kuv + V

E4315

j427 ua

H08A

H08MnA

HJ431 HlOMnSi Ar

200-300 ° C

760 ± 10 ° C

j427 ua

380 ° C 1.5 hli

Weld ntawm carbon steel thiab tsawg temp.low alloy steel

I + VI E4315

j427 ua

H08AH08MnA HJ431 HlOMnSi Ar

j427 ua

380 ° C 1.5 hli

 

Hlau No.

Joint niam txiv cov ntaub ntawv qeb qeb los yog pab pawg naj npawb

Hluav taws xob

SAW

GTAW

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe

Vuam ntawm high-strength low-alloy steels

II+ 11

E5015 j507 ua

H08MnA

HlOMnSi

HJ431

HlOMnSi

Ar

J507, J557

380-420 C

l 2 hnu

E5515-G

j507 ua

Vuam ntawm high-strength low-alloy steels

11+ (III-1) 11+ (III-2) E5015 j507 ua

H08MnA

H10Mn 2

HJ431

HlOMnSi

Ar

j507 ua

380 ° C

l 2 hnu

HJ350
(11 + 2) + (111 + 1) E5015 j507 ua

H10Mn 2

HJ431

J507, J557

(11 + 2) + (111 + 2)

E5515-G

j557 ua

HlOMnSi

HJ 35 O

380 ° C

l 2 hnu

Vuam ntawm lub zog qis-alloy steel thiab kub-resistant low-alloy steel

II + IV

E5003

j502 ua

150-250C

650-700 NwseC

j502 ua

150 ° C hli

E5015

j507 ua

150-250 ° C

650-700 ° C

j507 ua

38O°C1-2H kub

III + IV

E5003

j502 ua

150-250 ° C

650-700 NwseC

J 502 !50° Clh

E5015

j507 ua

j507 ua

380 ° C-2h

Vuam ntawm lub zog qis-alloy steel thiab kub-resistant low-alloy steel

II + V

E5015

j507 ua

200-300 ° C

760 ° C kub

10 ° C

j507 ua

380 ° C-2h

E5515-G

j557 ua

200-300 ° C

760 ° C ±

10eC

j557 ua

380 ° C 2 h

 

 

Hlau No.

Joint niam txiv cov ntaub ntawv qeb qeb los yog pab pawg naj npawb

Hluav taws xob

SAW

GTAW

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe

Lub zog qis-alloy steel thiab kub-resistant low-alloy steel

III + V

E5015

j507 ua

200-300 ° C

76 O ± IO ° C

J507J557

380-420 : kuveC

1.5h ib

E5515-G

j557 ua

nruab nrab ntawm tshav kub-resistant low-alloy steels

(IV-1) + (W-2) E5515-B1

R207

150-250 ° C

650-700 ° C

R207.R307

380-420 ° C

1.5h ib

E5515-B2

R307

E309-15 A307

A307

250 ° C 1.5h

IV + V

E5515-B1

R207

200-300 ° C

76 O ± IO ° C

R207.R307

R317.R407

38-420 NwseC

l 5 hnu

E5515-B2

R307

E5515-B2-V

R317

E6015-B3

r407 ua

E3I0-15 A407

A407

250 ° C 1.5h

Vuam ntawm pearlitic hlau thiab ferritic stainless hlau

(I + W) + VII

E309-16 A302

A302

150 ° C h

E309-15 A307

A307

250 ° C

 

Hlau No.

Joint niam txiv cov ntaub ntawv qeb qeb los yog pab pawg naj npawb

Hluav taws xob

SAW

GTAW

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe

Vuam ntawm pearlitic hlau thiab ferritic stainless hlau

1+ (vn-i)

E309-16 A302

HlCr24Nil3

HJ 260

HlCr24Nil3

Ar

150 ° C

lh

E309-15

A307

250 ° C

Ih

E309MO-16

A312

150 ° C

Ih

11+ (VII-1)

E309-I6

A302

HlCr24Nil3

HJ 260

HlCr24Nil3 Ar

150 ° C

Ih

E309Mo-16

A312

IH+ (vn-i)

E312-16

A402

HlCr26Ni2l Ar

150 ° C

Ih

E310-15

A407

250 ° C

Ih

 

Hlau No.

Joint niam txiv cov ntaub ntawv qeb qeb los yog pab pawg naj npawb

Hluav taws xob

SAW

GTAW

Pre Temp ua ntej weld

Temp.Tom qab weld

Vuam khoom kom qhuav Temp.

Qws

Hlau hlau No. (standard)

Flux

Hlau hlau No. (standard)

Roj

Qauv

Lub khw kos npe

Lub khw kos npe

Vuam ntawm pearlitic hlau thiab ferritic stainless hlau

IV+ (VD+1) E309-I6

A302

HlCr24Nil3

Ar

150 ° C

Ih

E310-16

A402

HlCr26Ni21

Ar

250 ° C

Ih

E310-I5

A407

HlCr26Ni21

Ar

150 ° C

Ih

E309-16

A302

HlCr24Nil3

Ar

E310-16

A402

HlCr26Ni21

Ar

E310-15

A407

HlCr26Ni2l

Ar

VI + (VD-1) E309-16

A302

HlCr24Nil3

Ar

150 ° C

Ih

E309-15

A307

250 ° C

ih


Post lub sij hawm: Mar-20-2023